ASTM A325 Bolts: Specification, Chemical Composition, Dimensions & Torque

ASTM A325 bolts are heavy hex structural bolts with a minimum tensile strength of 120 ksi, used to join steel members in buildings, bridges and towers. A325 now sits inside ASTM F3125 as Grade A325, and it comes in two types: Type 1 (carbon steel) and Type 3 (weathering steel).

If your mill certificate says A325 but your order says F3125, you are looking at the same grade under its current name. This guide covers the chemical composition and mechanical properties of both types, heavy hex dimensions, pretension and torque, compatible nuts and washers, and how A325 compares with A490. 

Unifit Fastener has supplied fasteners from India since 2014. Need A325 bolts for your project? Send us the size, quantity and finish, and we'll get back to you with a quote and test certificates.

Request a quote

What Is ASTM A325?

ASTM A325 is the specification for heavy hex structural bolts used to join steel members in buildings, bridges, towers and heavy equipment bases. The bolts are carbon steel bolts made from medium carbon steel (Type 1) or weathering steel (Type 3), quenched and tempered to a minimum tensile strength of 120 ksi in sizes from 1/2 to 1 1/2 inch. Head and thread dimensions follow ASME B18.2.6. As a structural grade, the material specifications and requirements come from ASTM F3125, not from the supplier.

Typical uses:

  • Steel framed buildings and bridges
  • Towers and masts
  • Heavy equipment bases

Are Stud Bolts and Threaded Rods Covered by A325?

No. A325 covers heavy hex bolts only. For stud bolts and threaded rod, look at ASTM A193 B7, A307 or F1554. See our ASTM A193 Grade B7 fasteners, and our stud bolts.

ASTM A325 vs F3125 Grade A325

ASTM A325 was withdrawn as a standalone standard in 2016. It was folded into ASTM F3125 and F3125M, together with A325M, A490, A490M, F1852 and F2280. What changed is the paperwork the requirements now live in F3125, and the larger sizes were aligned with the smaller ones. 

Old name

Current name

Note

A325

F3125 Grade A325

Inch series, 120 ksi minimum tensile

A325M

F3125M Grade A325M

Metric series, 830 MPa minimum tensile

F1852

F3125 Grade F1852

Twist off, tension control bolts

The grade kept its name and its 120 ksi minimum tensile strength. What changed is the paperwork: the requirements now live in F3125, and the larger sizes were aligned with the smaller ones.

ASTM A325 Types

Two types are in use. Type 2 was withdrawn, so you will not find it listed.

Type 1

Type 1 is medium carbon steel, which may be supplied as carbon boron steel or alloy steel. The bolts are quenched and tempered. It is the general purpose type and can be plain, painted or hot-dip galvanized.

Type 3

Type 3 is weathering steel. Copper, nickel and chromium let it form a stable, protective rust layer, so it suits unpainted weathering steel structures in outdoor exposure. Pair it with A563 DH3 or C3 nuts and F436 Type 3 washers.

Type

Steel

Corrosion behaviour

Typical use

Matching nut and washer

Type 1

Medium carbon, carbon boron or alloy steel

Needs paint or galvanizing in the weather

General structural steel

A563 Grade C, C3, D or DH nut, F436 washer

Type 3

Weathering steel with copper, nickel and chromium

Forms a protective layer in the atmosphere

Unpainted weathering steel structures

A563 DH3 or C3 nut, F436 Type 3 washer

ASTM A325 Chemical Composition

All values are heat analysis percentages.

Element

Type 1

Type 3, Composition A

Type 3, Composition B 

Carbon

0.30 to 0.52

0.33 to 0.40

0.38 to 0.48

Manganese

0.60 min

0.90 to 1.20

0.70 to 0.90

Phosphorus

0.035 max

0.035 max

0.035 max

Sulfur

0.040 max

0.040 max

0.040 max

Silicon

0.15 to 0.30

0.15 to 0.30

0.30 to 0.50

Boron

0.003 max

-

-

Copper

Not listed

0.25 to 0.45

0.20 to 0.40

Nickel

Not listed

0.25 to 0.45

0.50 to 0.80

Chromium

Not listed

0.45 to 0.65

0.50 to 0.80

Molybdenum

Not listed

Not listed

0.06 max

ASTM A325 Mechanical Properties

Property

Value

Tensile strength

120 ksi min (830 MPa for A325M)

Yield strength

92 ksi min (660 MPa for A325M)

Elongation

14% min

Reduction of area

35% min

Older mill certificates may show something different for large sizes. The legacy A325 listed 105 ksi tensile and 81 ksi yield for bolts from 1 1/8 to 1 1/2 inch. F3125 gives those larger sizes the same requirement as 1 inch and under, so the 120 ksi figure applies across the range. We mention the old numbers so you are not thrown when you match a certificate to a current order.

Hardness Requirements

F3125 Grade A325 bolts must fall between 25 and 34 HRC (253 to 319 HB). Hardness is tested per F3125 and recorded on the mill test report supplied with each order.

ASTM A325 Heavy Hex Bolt Dimensions Chart

The chart gives dimensions for heavy hex structural bolts to ASME B18.2.6, in inches. Thread length is 2 times the diameter plus 1/4 inch for bolts 6 inches and shorter, and 2 times the diameter plus 1/2 inch for longer bolts.

Nominal size

Threads per inch (UNC)

Width across flats

Head height H basic

Thread length, bolts 6 in and shorter

Thread length, longer bolts

1/2

13

7/8

5/16

1 1/4

1 1/2

5/8

11

1 1/16

25/64

1 1/2

1 3/4

3/4

10

1 1/4

15/32

1 3/4

2

7/8

9

1 7/16

35/64

2

2 1/4

1

8

1 5/8

39/64

2 1/4

2 1/2

1 1/8

7

1 13/16

11/16

2 1/2

2 3/4

1 1/4

7

2

25/32

2 3/4

3

1 3/8

6

2 3/16

27/32

3

3 1/4

1 1/2

6

2 3/8

15/16

3 1/4

3 1/2

Structural bolt heads are shorter than the heads of ordinary heavy hex bolts, so do not mix up the two charts. For more, see our hex bolt guide.

ASTM A325 Bolt Torque Chart

Before you reach for a torque chart, know this: pretension is what counts in a structural A325 joint, and torque is a poor way to measure it. Lubrication and thread condition change the tension you get for the same torque, so the minimum pretension table below is the one to design and inspect against.

Minimum pretension for A325 bolts

Nominal size

Minimum pretension (kips)

1/2

12

5/8

19

3/4

28

7/8

39

1

51

1 1/8

56

1 1/4

71

1 3/8

85

1 1/2

103

Indicative torque at those pretensions

The formula is T = K x D x P, where T is torque in foot pounds, D is the nominal diameter in feet (inches divided by 12) and P is the pretension in pounds (kips x 1,000). 

Nominal size

Torque, ft lb (K = 0.20)

Range, ft lb (K = 0.15 to 0.25)

1/2

100

75 to 125

5/8

198

148 to 247

3/4

350

262 to 438

7/8

569

427 to 711

1

850

637 to 1,062

1 1/8

1,050

788 to 1,312

1 1/4

1,479

1,109 to 1,849

1 3/8

1,948

1,461 to 2,435

1 1/2

2,575

1,931 to 3,219

Approved ways to tighten a structural joint:

  • Turn of nut: snug tighten, then rotate the nut by a set amount. The most common method.
  • Calibrated wrench: torque set from a daily test of the actual bolt lot.
  • Twist-off tension control bolts: the splined end shears off at the set tension.
  • Direct tension indicators: washers with protrusions that flatten as tension is applied.

Not sure which tightening method suits your joint? Read our bolt torque chart. guide for torque by size, or talk to our technical team.

Contact our team.

Recommended Nuts and Washers for A325 Bolts

Bolt

Nut

Washer

Type 1, plain

A563 Grade C, C3, D or DH

F436

Type 1, hot dip galvanized

A563 Grade DH, tapped oversize after galvanizing

F436 galvanized

Type 3

A563 DH3 or C3

F436 Type 3

Washer requirements depend on the tightening method and hole type, so check the RCSC Specification for your joint. For the parts themselves, see our hex nuts and washers.

ASTM A325 Bolt Head Markings

Every A325 bolt head carries the grade mark A325 and the manufacturer's symbol. Type 3 bolts carry a distinguishing mark as well. The exact pattern is set in the marking clause of F3125, so check it against your order when you inspect a delivery.

ASTM A325 vs A490

Property

A325

A490

Tensile strength

120 ksi min

150 to 173 ksi

Yield strength

92 ksi min

130 ksi min

Galvanizing

Allowed, on Type 1

Not permitted, because of hydrogen embrittlement

Typical use

General structural

Higher load and heavily loaded joints

Types

1 and 3

1 and 3

Choose A325 unless the design calls for A490. Never swap in A490 where galvanizing is required. For a wider view of strength classes, see our high tensile fasteners page and our guide to grade 8.8 vs 10.9 vs 12.9 bolts.

Frequently Asked Questions

A325 bolts have a minimum tensile strength of 120 ksi (830 MPa for the metric A325M series) and a minimum yield strength of 92 ksi. They are made in Type 1 and Type 3, and the same strength applies from 1/2 to 1 1/2 inch.

A325 is the inch series. A325M is the metric series, from M16 to M36, with a minimum tensile strength of 830 MPa. Both now sit inside ASTM F3125, as Grade A325 and Grade A325M.

Yes. Type 1 can be hot dip galvanized to ASTM F2329, with an overtapped DH nut. Type 3 is weathering steel and is not normally galvanized. A490 bolts must not be hot dip galvanized because of hydrogen embrittlement.

Use an A563 Grade DH nut with an F436 washer. Grades C, C3, D and DH3 are also listed for A325, depending on the type and coating. Galvanized bolts take an overtapped DH nut.

Conclusion 

ASTM A325 bolts are 120 ksi heavy hex structural bolts, now specified as Grade A325 in ASTM F3125, in Type 1 for general use and Type 3 for unpainted weathering steel. Order by the full F3125 designation, match the nut and washer to the type and coating, and judge a joint by pretension rather than torque alone. Choose A490 only where the design needs it, and never galvanize it.

Planning a structural bolting job? Read our bolt torque chart guide, or Contact Unifit Fastener with your size, type and coating.